Two shops receive the same part drawing. One clears first article inspection after a single sample run, the other reworks the cavity for three months. The gap seldom lies in the part itself. It lies in a handful of numbers in MIM tooling design.
From feedstock flow to sintering, the cavity sets the shape of the green part and the dimensional chain that follows. Yujiaxin Tech starts every project with the metal injection molding process overview. This guide gives the formulas and parameter ranges engineers can apply at the drawing stage.
Key takeaways
- Size the cavity with the factor 1 / (1 - shrinkage), then correct locally for wall thickness.
- Place gates at thick sections, away from datum faces and cosmetic surfaces.
- Keep vent depths at 0.02 to 0.05 mm so gas escapes without flashing.
- Use 0.5 to 3 degrees of draft and support the green part with broad ejector pads.
- Choose H13 or S7 for production tools and hold mold temperature within ±1°C.
A plastic mold treats the cavity as the finish line. MIM tooling design treats the sintered part as the starting point and works backward. Feedstock fills the cavity as a green part, then loses 15% to 20% of its linear size during debinding and sintering. One tool must serve both stages, so the brief starts with final tolerance rather than cavity geometry.
Part manufacturability and tool construction are separate questions. Wall thickness, corner radii and holes belong to MIM part design guidelines. Cavity layout, gates, vents and ejection belong here. Confusing the two is the fastest route to a tool that cannot hold tolerance.
Every 0.01 mm of cavity error reaches the sintered part at roughly the same ratio. The error budget therefore belongs at the tool, not at the furnace.
The first pass uses one equation: scale factor = 1 / (1 - shrinkage). For 316L, linear shrinkage of 16% to 18% gives a factor of 1.19 to 1.22. For 17-4PH, shrinkage of 17% to 19% gives 1.21 to 1.24.
| Material | Linear shrinkage | Cavity scale factor |
|---|---|---|
| 316L | 16% to 18% | 1.19 to 1.22 |
| 17-4PH | 17% to 19% | 1.21 to 1.24 |
| Fe-2Ni | about 18% | about 1.22 |
| Ti-6Al-4V | about 15% | about 1.18 |
Uniform scaling solves only the first order problem. Thick to thin transitions cool at different rates, and shrinkage is not equal in every direction. Local correction follows a measured dilatometry curve, not an average catalog value. Critical bores can carry 0.05 to 0.10 mm of CNC stock so the tool holds the shape and machining holds the position.
The mechanism of sintering shrinkage is covered in the MIM process chain. This section stays with MIM tooling design: write measured shrinkage back into cavity coordinates, measure first articles on a CMM, then cut one correction pass. That loop closes the factor.
Place the gate at the thickest section so holding pressure reaches the area that shrinks most. Keep it off datum faces and visible surfaces. A gate that is too small freezes early, while an oversized gate leaves a mark and adds finishing time.
Balance runners geometrically in multi cavity tools and use cold slugs to trap the cooled front. Otherwise density differs from cavity to cavity and becomes a size difference after sintering.
Trapped gas and weld lines have root causes described in MIM defect analysis. Design prevention in MIM tooling design means putting vents at the end of fill and where flow fronts meet. Vent depth runs 0.02 to 0.05 mm, adjusted at trial against the actual fill pattern.
Green parts are far weaker than sintered ones. Draft of 0.5 to 3 degrees is normal, with the larger value for fine teeth and deep holes. Put ejector pins on stiff sections and prefer broad pads over slender pins to avoid whitening and micro cracks.
The parting line across a cosmetic face leaves a witness mark. Inserts turn an undercut into a removable side action. MIM tooling design also fixes the extra steel left for future changes at this stage, because adding an insert later can mean rebuilding the whole cavity.
Prototype work can use P20 for speed. Production tools usually use H13 or S7 at 48 to 52 HRC after heat treatment, with carbide inserts for very long runs. Material and heat treatment choices can be checked against MPIF standards and the ASM International material handbook.
Hold mold temperature between 80°C and 120°C and keep fluctuation within ±1°C so green part stress stays stable. Water lines should sit at an even distance from the cavity. Cavity to cavity temperature differences turn directly into dimensional spread.
Wear changes cavity size slowly, so MIM tooling design should set the regrind interval and the insert replacement point in advance. Measure critical dimensions on each first article and track them with SPC. When drift passes one third of the tolerance band, schedule maintenance before scrap appears.
How is the scale factor in MIM tooling design calculated? Use 1 / (1 - shrinkage), then correct it with shrinkage measured on the first articles. A generic supplier multiplier is a starting guess, not a final number.
Is shrinkage a fixed value? No. Alloy, wall thickness and the sintering cycle all move it, and one tool can show different values in different regions.
How do multi cavity tools stay consistent? Balance runners geometrically, hold temperature uniformly, and number every cavity with its own dimension record.
When does a critical feature need machining stock? When tolerance is tighter than 0.02 mm or the feature mates with another part, MIM holds the shape and machining holds the location.
A prototype tool answers whether the geometry fills. A production tool answers whether it still holds tolerance after ten thousand shots. MIM tooling design is where that second question gets priced, through steel choice, vent depth and a regrind plan written before the first cut.
For context, read MIM compared with investment casting. Yujiaxin Tech runs an ISO 9001 system and serves military projects. Ask about a MIM tooling design proposal and our engineers complete a DFM review before steel is cut.